# TC200 Thermal Cycling: What Fails Between -40 and +85

> Thermal cycling to IEC 61215-2 MQT 11: why 200 cycles between -40 and 85 C fail solder joints, and what the powered ramp actually changes.

![TC200 Thermal Cycling: What Fails Between -40 and +85](https://cdn.ooitech.com/static/upload/image/20261026/thermal-cycling-tc200-failure-modes.png)

- ** Ooitech Editorial Team
- ** 2026-11-17
- ** 0 Views
- ** [Photovoltaics & Applications](./Photovoltaics.html)

Editorial responsibility for this article rests with **Wuhan Ooi Photoelectric Technology Co., Ltd.** Written and reviewed by the Ooitech editorial team. See our [editorial policy](/editorial-policy.html) for how we write, where AI tools are used, and how to request a correction.

## TC200 Thermal Cycling: What Fails Between -40 and +85

**Quick answer:** TC200 is a sequencing test before it is a severity test. IEC 61215-2 MQT 11 runs 200 cycles between -40 °C ± 2 and +85 °C ± 2, about 6 h each, with ramps capped at 100 °C/h and at least 10 min of dwell at both ends. The detail that decides what fails is the current schedule: Imp ± 2 % flows only while the module climbs from -40 to +85, and drops below Imp × 1 % during the hot dwell, the cooldown and the cold dwell. Solder joints are therefore loaded while thermal expansion is already moving them, with Joule heating and recombination stress arriving on top. 200 cycles is 200 low-cycle fatigue loads shared across every interface bonded into one laminate, and the damage collects at ribbon-to-busbar joints, busbar jumps and cell edges. Chamber setup, not the wording of the clause, is where most of this test goes wrong.

A module that passes 200 cycles can still carry a joint that is most of the way consumed. The result is pass or fail, with no margin attached to it.

## The current schedule decides the failure mode

Two modules can sit in the same chamber, see the same 125 K swing, and fail differently because of how the current was applied. Temperature sets the amplitude of the stress. **The schedule decides which interface absorbs it.**

MQT 11 asks for forward current at Imp ± 2 % while the module heats from -40 to +85. Everywhere else the current falls below Imp × 1 %: the hot dwell, the cooldown, the cold dwell. Read that as a statement about where the standard expects damage to happen, because that is what it is.

During our thermal chamber runs, we synchronize the programmable power supply to deliver forward current within Imp ± 2 % from -40 to +85, dropping below Imp × 1 % immediately upon reaching the dwell.

The two tests pull in opposite directions. DH1000 works on encapsulant and metallization chemistry over 1,000 h at 85 °C and 85 % RH; TC200 works on mechanical joints across some 1,200 h of cycling. A module can pass one and fail the other, and laboratories that file both as generic environmental testing misread the certificate. The [DH1000 failure modes](https://www.ooitech.com/dh1000-damp-heat-test-failure-modes-and-mechanisms.html) article covers the other half of that pair.

## What MQT 11 specifies, in the numbers that matter

| Parameter | Value | What it controls |
| --- | --- | --- |
| Cold extreme | -40 °C ± 2 °C | Lower end of the strain cycle, and metal ductility |
| Hot extreme | +85 °C ± 2 °C | Upper end, plus encapsulant creep rate |
| Cycles | 200 | Full strain reversals |
| Cycle time | about 6 h typical, about 2.8 h at the limit | Throughput, and hours at temperature |
| Ramp rate | no faster than 100 °C/h | Through-thickness gradient, and the shortest legal cycle |
| Dwell | at least 10 min at each extreme | Whether the laminate core reaches setpoint |
| Current on the -40 to +85 ramp | Imp ± 2 % | Joule heating at peak relative motion |
| Current in other segments | below Imp × 1 % | Separates creep from self-heating |
| Junction box load, recent editions | 5 N | Cable pull on the box and its adhesive |
| Pass criteria | no severe visual defect, insulation and wet leakage pass, power loss 5 % or less | End point, not a margin |

Source: IEC 61215-2, MQT 11. The 6 h figure is typical for a loaded chamber; 2.8 h is the floor the ramp and dwell limits allow.

One cycle in two lanes: 125 K of swing above, current at Imp only while the module climbs, below Imp × 1 % for the hot dwell, the cooldown and the cold dwell.

TC200 is one line in a longer qualification list, and the line that loads metal rather than chemistry. The comparison with cell-level and module-level causes is set out in this [list of PV module reliability tests](https://www.ooitech.com/pv-module-reliability-tests-list-cell-vs-module-failure-causes.html).

## Why the powered ramp does the damage

Start at -40. The solder is stiff, the encapsulant has hardened toward a glassy state, and the copper ribbon has contracted more than the silicon under it. Nothing is moving yet. Then the chamber ramps, and every interface in the stack begins to shear at once.

At that same moment, current at Imp enters the string. A joint with contact drop becomes a local heat source inside a structure whose two sides are already expanding at different rates. The cell dissipates power too, so it runs slightly above the chamber setpoint, and the joint sees a larger amplitude than the thermocouple reports.

The clause is not trying to make the ramp hotter. It is making it coincident: **expansion is moving the joint while current is loading it**, so both damage contributions land in the same window. That is why weak joints surface within 200 cycles here, while a thermal soak of the same amplitude can run far longer before the same joint announces itself.

## Why the unpowered segments matter just as much

The hot dwell is where the encapsulant decides whether it will stay bonded. At +85 °C the polymer softens and creeps, peel strength falls, and the interface moves under load rather than resisting it. With current off, temperature is the only thing driving that creep, so the exposure is a soak measured in hours instead of a self-heating experiment. The [line-shaped bubbles along the ribbons](https://www.ooitech.com/epe-encapsulant-lamination-delamination-line-shaped-bubbles-along-solar-cell-ribbons.html) are the same mechanism seen from the laminate side.

The cooldown is where the shear reverses. Everything pushed one way on the ramp is pulled back, and at the cold end the copper has hardened and lost ductility, which is the moment a weakened ribbon can crack. Cooling under current would put modules at different operating points as temperatures diverge, and mismatch losses would turn into local hot cells: an uncontrolled stress stacked on the one being measured.

There is a measurement reason too. I-V and EL readings are taken unpowered and at a known temperature, so the hot dwell and the cold dwell are the only points in a cycle where a reading can be compared with the same reading 200 cycles later. Power the dwells and the reference state disappears.

So the four segments do four jobs. The ramp loads the joints, the hot dwell works adhesion under creep, the cooldown reverses the shear, the cold dwell hardens the metal and supplies the measurement point. **Three of the four are unpowered on purpose.**

## The CTE chain: 9, 3, 17, 23 ppm/K in one laminate

One laminate holds four materials with four expansion coefficients bonded into one body: soda-lime glass near 9 ppm/K, silicon about 2.6 ppm/K in the source data (it rounds to 3), copper ribbon near 17 ppm/K and an aluminum frame near 23 ppm/K. The encapsulant is above 100 ppm/K, which is why it buffers the stack rather than carrying load.

Across the 125 K swing, each pair accumulates displacement in proportion to its difference. Glass against silicon is 6 ppm/K apart. Silicon against copper is 14 ppm/K apart, the largest mismatch sitting directly on a cell.

Take a 182 mm cell edge, a 125 K swing and 14 ppm/K between ribbon and silicon: relative movement comes to about 0.32 mm, for illustration. That displacement does not vanish; a solder layer 10 to 25 &micro;m thick absorbs it, which is why the joint behaves as a low-cycle fatigue specimen and not an elastic connection. Whether it has anywhere to go depends on the bond around it, and a laminate that left the [laminator](https://www.ooitech.com/single-layer-double-chamber-automatic-bipv-laminator-otcy-2754dd-ooitech-solar-panel-lamination-equipment.html) with voids along the ribbon rows has spent part of its compliance already.

Solder fatigue follows a power law in strain amplitude, with an exponent near 2 for common tin-lead and tin-silver-copper alloys, so a swing 10 % larger costs more than 10 % of life. It also explains why the cold end earns its place: -40 °C is where the copper is stiffest and the mismatch is resolved against a solder with very little left to give.

## Where it breaks: joints, busbar jumps, cell edges

### Solder joints and the intermetallic layer

The ribbon-to-busbar joint is the first place to look. Under repeated shear the solder grain structure coarsens, stress concentrates at the grain boundaries, a microcrack opens and runs along the solder layer until the joint is high-resistance or open. Low-temperature alloys containing bismuth are especially prone to that coarsening, and none of it is visible from outside. Where the [ribbon manufacturing process](https://www.ooitech.com/how-pv-ribbon-is-made-drawing-annealing-and-tinning.html) leaves a soft or uneven coating, the solder has less to work with from day one.

### Busbar jumps and ribbon crossovers

Where a ribbon leaves one cell and crosses to the next, the fillet changes shape, the constraint changes, and the same displacement is forced through a shorter, less compliant length. These joints open early in EL as short dark segments, and they survive a pull test, because a pull test does not reverse direction 200 times.

### Cell edges and laser-cut damage

Silicon fails in tension, and the tension arrives at the edges. A laser-cut edge, a scribe line from half-cell separation, or a microcrack left by stringing is a stress raiser. When the ribbon contracts and pulls on the cell, stress intensity at that tip rises past the fracture toughness of silicon, and the crack grows into the branch pattern EL shows as dark lines and snail trails. The source note is blunt: TC200 audits process damage, because a crack invisible at incoming inspection will propagate.

### Junction box and bypass diode

The box carries current while it sits through the temperature schedule. Potting compound and base adhesive crack under thermal stress, the box lifts from the backsheet, and the bypass diode sees junction excursions that repeated cycling turns into package damage or thermal runaway. Recent editions add a 5 N load to represent cable pull, planting a mechanical test on top of a thermal one.

## Reading the electrical signature

The I-V parameters separate the two failure families more cleanly than visual inspection does.

| Parameter | Interconnect or joint failure | Cell-level crack or shunt |
| --- | --- | --- |
| Rs | clearly up | slightly up |
| Rsh | essentially unchanged | clearly down |
| FF | clearly down | clearly down |
| Voc | essentially unchanged | clearly down |
| Isc | essentially unchanged | clearly down |
| EL | dark lines or patches at joints, a whole string dark in severe cases | line, branch or snail-trail patterns |
| Visual | ribbon detachment or alloy separation in severe cases | often nothing to see |

Read the first two rows together. Resistance up with shunt resistance flat is a joint problem, and the fix lives in soldering, ribbon specification and lamination pressure. Shunt resistance and open-circuit voltage both falling is a silicon problem, and no rework recovers it.

EL moves before either number does. A joint that has started to crack shows a dark segment at the joint long before series resistance shifts enough to trip the 5 % power criterion, which is how a module passes the clause while carrying a joint that is nearly spent.

## Six hours versus 2.8 hours: what compression costs

The 2.8 h figure is not arbitrary. Two ramps of 125 K at the 100 °C/h cap take 2.5 h, and two 10-minute dwells add 0.33 h, which comes to 2.83 h. That is the floor the clause permits, and a chamber running at the floor has nothing left in reserve.

A typical 6 h cycle spends the difference on the laminate core instead of the air, and on ramps the chamber can hold while carrying a load.

| Aspect | Typical 6 h cycle | Compressed 2.8 h cycle |
| --- | --- | --- |
| Ramp rate | well under the cap, set by chamber capacity under load | at the cap, 1.25 h per ramp |
| Dwell at each extreme | long enough for the core to stabilize | 10 min minimum, often surface only |
| Hours at +85 °C | hours per cycle, so creep is represented | minutes, so creep is under-represented |
| Gradient through the laminate | small, close to isothermal | larger, so joints see a harsher local swing |
| Failure modes exercised | joint fatigue plus encapsulant creep | joint and edge-crack screening, weak on adhesion |
| Appropriate use | type approval and lifetime claims | incoming audits, process comparison, gross defects |

Compression is legitimate only if module temperature is logged rather than chamber air. A 10 min dwell that satisfies the clause on paper can leave the core short of setpoint in a loaded chamber, and the amplitude then shrinks quietly.

To prevent temperature lag across loaded racks, we monitor module backsheet sensors directly and trigger the 10 min dwell timer only when the internal laminate reaches the actual test setpoint.

## Where the test goes wrong: inside the chamber

Most arguments about TC200 concern clause wording. Most surprises concern hardware.

- Fixtures. Clamping the frame elsewhere changes the constraint path; over-clamping holds the module flat while the laminate tries to move, removing the displacement the test exists to apply.
- Current leads. Two-wire connection puts lead resistance in series with the string. A warm tab at the feedthrough is a bad joint outside the module that reads as a module failure.
- Thermocouples. Sensing chamber air instead of the backsheet is the commonest error here; air tracks setpoint while the laminate lags, turning the recorded cycle into fiction.
- Chamber capacity. A chamber that reaches -40 °C empty may not hold +85 °C with 20 modules dissipating power on the ramp; the result is a slow ramp or a setpoint that never arrives, and both report as a pass.
- Condensation. Frost on the frame at the cold end is routine and belongs in no record.

None of that is in the clause, because the clause cannot know your fixture. It is also the first thing an auditor looks at, and the fastest way to tell a laboratory that ran the test from one that ran a program.

## Where these numbers come from

Conditions, tolerances, current schedule, ramp cap, dwell, junction box load and pass criteria come from IEC 61215-2, MQT 11, as summarized in a Chinese technical note on TC200 that this article is built from. Copper at 17 ppm/K, silicon at 2.6 ppm/K, the 10 to 25 &micro;m solder thickness and the encapsulant figure above 100 ppm/K come from the same note.

Glass at about 9 ppm/K and aluminum at about 23 ppm/K are standard handbook values, quoted to one significant figure, which is all the comparison needs. The 0.32 mm displacement is arithmetic on a 182 mm cell edge across 125 K, for illustration, not a measured value. The 2.83 h floor is arithmetic on the clause limits. The fatigue exponent near 2 is the textbook Coffin-Manson value for solder, not something MQT 11 states.

Chamber-side items in the previous section are setup checks drawn from how these systems are commissioned, not statistics. Where this article says a module can pass one test and fail another, that is a claim about what each test loads, not a failure rate. The note gives no population data, so none is quoted here.

## Questions engineers ask about TC200

### Q: Why 200 cycles and not 50?

Because the damage is cumulative and the interesting failures arrive late. Solder fatigue is a power law, so the last few hundred cycles do most of the work. 200 is the compromise between catching a weak joint and spending seven weeks of chamber time per sample.

### Q: Is -40 to +85 realistic for a real site?

As air temperature, +85 °C is above what most sites deliver, though a dark module at noon in still air runs far above ambient. -40 °C is ordinary in continental and high-altitude locations. The pair is an accelerated envelope, not a weather record, and cells run hotter than the backsheet, which widens the real swing.

### Q: Can a lab run 2.8 h cycles for qualification?

The clause allows compression inside its limits, but the load has to follow. A report that states 200 cycles without stating cycle time hides whether the module spent hours at +85 °C per cycle or minutes, and those are different tests under the same name.

### Q: Why Imp and not Isc?

Imp is the current a module passes through most of its working life, so it is the heat load that belongs in the test. Isc would overstate heating at the hot end without adding information about the joint.

### Q: Which reading moves first?

EL, in almost every case. A joint that has begun to crack shows a dark segment at the joint before series resistance moves enough to matter. Rs and FF then confirm what the image already showed.

### Q: Does passing TC200 predict field life in a hot climate?

Partly. It predicts joint behavior well, since that is what the current schedule loads. It says less about encapsulant creep and hydrolysis, which belong to damp heat, and less about the daily low-amplitude cycling a field module sees.

### Q: What is the 5 N junction box load for?

It represents cable pull on the box and its adhesive, applied during the thermal schedule so the adhesive is worked while it is hot and soft. A small load applied at the worst moment is the whole idea.

### Q: TC200 or DH1000 first?

Both, and in that order if there is one chamber. TC200 finds the mechanical defects that make a module unfit to be tested further, and damp heat needs 1,000 h to say anything about chemistry.

## Final thoughts

Thermal cycling gets described as 200 trips between two temperatures. The trips are the easy part to program and the least useful part to argue about. What decides the outcome is that current flows while the joints are moving, that three segments are deliberately unpowered, and that the chamber, the fixture and the thermocouple do as much of the work as the clause does.

After thermal cycling exposes mechanical strains in your laminate, electrical dielectric checks verify package safety. We supply the [CHT9980A and CHT9981A safety testers](https://www.ooitech.com/cht9980a-cht9981a-pv-safety-comprehensive-tester-solar-panel-hipot-insulation-ground-continuity-tester.html) for hipot, insulation resistance, ground continuity, and wet leakage testing. Send your drawings, module stack, or production samples to our engineering team for evaluation.

---

##### Tags :

![](/template/ooitech/assets/img/shape/06.png)

![](https://cdn.ooitech.com/runtime/image/w800_h700_fitblur_v2_w800_h700_fitblur_v2_1757399770541443.webp)

### Request A Quote

All uploads are secure and confidential.

## We deliver expertise you can trust our service

Direct-from-Factory Equipment.

![](/template/ooitech/assets/img/icon/money-2.svg)

### Cost-Effective Advantages

We deliver exceptional value, maximizing results while optimizing budgets for clients.

![](/template/ooitech/assets/img/icon/staff.svg)

### Our Experience Team

Our skilled professionals specialize in innovative solutions and tailored strategies.

![](/template/ooitech/assets/img/icon/certified.svg)

### 15+ Years Industry Experience

Deep expertise ensures reliable, trend-aware, and proven outcomes for success.

![](https://cdn.ooitech.com/static/upload/image/20250910/1757477357667605.webp )

![](https://cdn.ooitech.com/static/upload/image/20250910/1757477724911512.webp)

![](/template/ooitech/assets/img/shape/06.png)

## What Our Client Say's about us

Client testimonials praise our deep understanding of their challenges, which leads to innovative solutions and strong ROI. Long-term collaborations—some over a decade—demonstrate their trust and satisfaction. Their success stories drive us to continually exceed expectations. [Know More **](#quote-form)

![](/template/ooitech/assets/img/icon/quote.svg)

A man with a big soul. Thank you very much for your visit Mr Wu. Thank you very much for the services provided in installing equipment and training my students. The kindest person and professional in his field

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026041716444445.webp)

### Jizzakh Polytechnic Institute

![](/template/ooitech/assets/img/icon/quote.svg)

Thanks to Ooitech for providing highly suitable BC solar cell experimental equipment.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1776426122864564.webp)

### KTECH

![](/template/ooitech/assets/img/icon/quote.svg)

thank you for ooitech's professional support and on time after service.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1784509010217979.webp)

### Diarra From Africa

![](/template/ooitech/assets/img/icon/quote.svg)

Thanks to Ooitech for providing the fully automated production equipment—your installation and after-sales service have been excellent.

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026041720921238.webp)

### Amjad

![](/template/ooitech/assets/img/icon/quote.svg)

Thank you again so much again for the very big big help for improving and fixing the factory and also teaching the workers how to use the machines

![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1757479675272137.webp)

### Mark

BIPV Philippines

## Our Latest Products

![SC-10C Silicon Wafer Laser Cutting Machine](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774340166130021.webp)

- [** ooitech](./SC-10C-Full-Automatic-Silicon-Wafer-Laser-Cutting-Machine-High-Precision-Solar-Cell-Production-Equipment.html)
- [** 30246](./SC-10C-Full-Automatic-Silicon-Wafer-Laser-Cutting-Machine-High-Precision-Solar-Cell-Production-Equipment.html)

### SC-10C Silicon Wafer Laser Cutting Machine

SC-10C Full Automatic Silicon Wafer Laser Cutting Machine by Ooitech - High-speed precision cutting equipment for solar cell production with 860PCS/H

![Solar Cell Laser Cutting Machine — OLS-20E Dual Laser](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026031858869524.webp)

- [** ooitech](./OLS-20E-Full-Automatic-Solar-Cell-Laser-Scribing-and-Breaking-Machine-High-Precision-Solar-Panel-Manufacturing-Equipment.html)
- [** 27276](./OLS-20E-Full-Automatic-Solar-Cell-Laser-Scribing-and-Breaking-Machine-High-Precision-Solar-Panel-Manufacturing-Equipment.html)

### Solar Cell Laser Cutting Machine — OLS-20E Dual Laser

Solar cell laser cutting machine for shingled cells: OLS-20E runs two laser heads with automatic 1/4 break, cutting kerf loss and micro-cracks on MBB.

![Solar Panel Layup and Bussing Machine: 10W to 600W Modules, TOPCon BC PERC HJT](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1790216004194913.webp)

- [** ooitech](./solar-panel-layup-and-bussing-machine.html)
- [** 373](./solar-panel-layup-and-bussing-machine.html)

### Solar Panel Layup and Bussing Machine: 10W to 600W Modules, TOPCon BC PERC HJT

Solar panel layup and bussing machine in six models, SAW-100A to SAW-600A, for 10 W to 600 W modules: high-frequency bus ribbon soldering, 15 s per group, inline or standalone.

![Solar Panel Making Machine: Choosing Your First Line](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774942832346689.webp)

- [** ooitech](./solar-panel-making-machine.html)
- [** 126](./solar-panel-making-machine.html)

### Solar Panel Making Machine: Choosing Your First Line

Buying your first solar panel making machine: the 9 build steps, semi-automatic vs automatic, staffing, facility needs and quotation checks.

![OEL-S2400 Solar Panel EL Tester: 4928 x 3264px](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774351284414161.webp)

- [** Rachael](./solar-panel-el-defect-tester-oel-s2400-electroluminescence-testing-machine-for-solar-module-quality-inspection.html)
- [** 60900](./solar-panel-el-defect-tester-oel-s2400-electroluminescence-testing-machine-for-solar-module-quality-inspection.html)

### OEL-S2400 Solar Panel EL Tester: 4928 x 3264px

Ooitech OEL-S2400 Solar Panel EL Defect Tester is an offline electroluminescence testing machine designed to detect microcracks, black spots

![Low-Temperature PV Ribbon and Flux for Solar Strings](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026032717287347.webp)

- [** Rachael](./Solar-Panel-Soldering-Ribbon-and-Flux-Essential-Components-for-PV-Module-Manufacturing.html)
- [** 21302](./Solar-Panel-Soldering-Ribbon-and-Flux-Essential-Components-for-PV-Module-Manufacturing.html)

### Low-Temperature PV Ribbon and Flux for Solar Strings

PV ribbon and flux for solar cell interconnection: low-temperature soldering ribbon in high-purity tin-coated copper, supporting MBB and half-cut lines.