    "schemaVersion": "ooitech-article.v1",
    "url": "https://www.ooitech.com/sinx-too-thin-and-silver-paste-punches-through-the-poly-layer-too-thick-and-contact-resistance-jumps-600x-isfh-points-to-a-fix.html",
    "language": "en",
    "title": "SiNx Too Thin and Silver Paste Punches Through",
    "description": "An ISFH study on POLO contacts shows how backside SiNx capping thickness and firing temperature must be paired to keep contact resistance low without",
    "keywords": "SiNx capping layer, POLO contact, contact resistivity, etch pits, firing temperature, TOPCon",
    "ogType": "website",
    "image": "https://cdn.ooitech.com/static/upload/image/20260715/ffe27327c3b76ab63793c7ff5e44c617.webp",
    "headings": [
        {
            "level": 1,
            "text": "SiNx Too Thin and Silver Paste Punches Through"
        },
        {
            "level": 2,
            "text": "SiNx Too Thin and Silver Paste Punches Through"
        },
        {
            "level": 2,
            "text": "Product Introduction"
        },
        {
            "level": 2,
            "text": "Technical Parameters"
        },
        {
            "level": 3,
            "text": "How the experiment was set up"
        },
        {
            "level": 3,
            "text": "All samples fired at 800°C, only rear SiNx thickness varied"
        },
        {
            "level": 3,
            "text": "Firing temperature scan on 55nm and 60nm samples"
        },
        {
            "level": 2,
            "text": "Technical Advantages"
        },
        {
            "level": 3,
            "text": "First finding: too thick and the paste can't fire through"
        },
        {
            "level": 3,
            "text": "Second finding: thickness and temperature are paired"
        },
        {
            "level": 3,
            "text": "The mechanism: etch pit size is the key"
        },
        {
            "level": 2,
            "text": "Product Application"
        },
        {
            "level": 3,
            "text": "What can a production line actually use?"
        },
        {
            "level": 3,
            "text": "Three things the paper didn't say"
        },
        {
            "level": 3,
            "text": "Reading it together with JA Solar 2016"
        },
        {
            "level": 3,
            "text": "A reminder for the line: don't only stare at poly when hunting for efficiency loss"
        },
        {
            "level": 3,
            "text": "Ooitech's View"
        },
        {
            "level": 2,
            "text": "References"
        },
        {
            "level": 2,
            "text": "Further reading and background data"
        },
        {
            "level": 5,
            "text": "Tags :"
        },
        {
            "level": 5,
            "text": "Table of Contents"
        },
        {
            "level": 5,
            "text": "Category"
        },
        {
            "level": 5,
            "text": "Related Posts"
        },
        {
            "level": 6,
            "text": "TOPCon Solar Cell Manufacturing Process: Step-by-Step"
        },
        {
            "level": 6,
            "text": "Solar Stringer Machine: How Tabber Stringers Work"
        },
        {
            "level": 6,
            "text": "Triple-Junction GaAs Solar Cell — Structure and Gains"
        },
        {
            "level": 6,
            "text": "26.2% Certified Efficiency Breakthrough"
        },
        {
            "level": 6,
            "text": "33.25% Efficiency, 96% MPPT Retention After 1000 Hours:"
        },
        {
            "level": 5,
            "text": "Recent Post"
        },
        {
            "level": 6,
            "text": "BC Stringing Warp: Both Ends Curl, Five Levers to Fix It"
        },
        {
            "level": 6,
            "text": "BC Orders Booked to 2027: What It Changes for a Module Line"
        },
        {
            "level": 6,
            "text": "PV Encapsulant Film: EVA, White EVA, POE, EPE and Beyond"
        },
        {
            "level": 5,
            "text": "Popular Tags"
        },
        {
            "level": 3,
            "text": "Request A Quote"
        },
        {
            "level": 2,
            "text": "We deliver expertise you can trust our service"
        },
        {
            "level": 3,
            "text": "Cost-Effective Advantages"
        },
        {
            "level": 3,
            "text": "Our Experience Team"
        },
        {
            "level": 3,
            "text": "15+ Years Industry Experience"
        },
        {
            "level": 2,
            "text": "What Our Client Say's about us"
        },
        {
            "level": 3,
            "text": "Amjad"
        },
        {
            "level": 3,
            "text": "Diarra From Africa"
        },
        {
            "level": 3,
            "text": "KTECH"
        },
        {
            "level": 3,
            "text": "Mark"
        },
        {
            "level": 3,
            "text": "Jizzakh Polytechnic Institute"
        },
        {
            "level": 2,
            "text": "Our Latest Products"
        },
        {
            "level": 3,
            "text": "SS-1500B Solar Cell Tabber Stringer: 1200 Cells/h"
        },
        {
            "level": 3,
            "text": "OPT-S110H Offline String EL Tester: ≤2s, 4.6MP"
        },
        {
            "level": 3,
            "text": "OEL-S2400 Solar Panel EL Tester: 4928 x 3264px"
        },
        {
            "level": 3,
            "text": "Solar Panel Sealant and Tape: Silicone, Butyl, PET"
        },
        {
            "level": 3,
            "text": "KS-01C Junction Box Welding Machine: 16s Cycle"
        },
        {
            "level": 3,
            "text": "SS-2500B Tabber and Stringer: 2400 Cells/h, 3-20BB"
        }
    ],
    "wordCount": 2897,
    "markdown": "# SiNx Too Thin and Silver Paste Punches Through\n\n> An ISFH study on POLO contacts shows how backside SiNx capping thickness and firing temperature must be paired to keep contact resistance low without\n\n![SiNx Too Thin and Silver Paste Punches Through](https://cdn.ooitech.com/static/upload/image/20260715/ffe27327c3b76ab63793c7ff5e44c617.webp)\n\n- ** Jerry\n- ** 2026-07-15\n- ** 901 Views\n- ** [Blog](./Blog.html)\n\nEditorial responsibility for this article rests with **Wuhan Ooi Photoelectric Technology Co., Ltd.** Written and reviewed by the Ooitech editorial team. See our [editorial policy](/editorial-policy.html) for how we write, where AI tools are used, and how to request a correction.\n\n## SiNx Too Thin and Silver Paste Punches Through\n\n**Quick answer:** Front-film silicon nitride on a TOPCon cell has to satisfy two opposing requirements, and the thickness that satisfies both is narrow. The SiNx layer acts as the anti-reflective coating, so a thicker film improves optical performance up to a point. It also has to withstand the firing step and prevent the silver paste from punching through to the silicon during contact formation. Coat it too thin and silver penetrates the emitter, causing shunts; coat it too thick and the paste fails to form a proper contact, raising contact resistance. Working thicknesses in production sit in the 40 nm to 80 nm band, with firing peaks around 790 °C to 800 °C. The interaction is why paste formulation and firing profile are developed together with the coating recipe rather than independently.\n\nPV Module Manufacturing · by Jerry, Ooitech\n\n## Product Introduction\n\nAnyone running a [TOPCon](https://www.ooitech.com/what-is-topcon-solar-cell-a-complete-guide-to-tunnel-oxide-passivated-contact-technology.html) process line has faced this bind. Coat the SiNx too thin and you worry the silver paste burns through the passivation layer, dragging Voc down. Coat it too thick and contact resistance shoots up, and FF can't hold. Thin scares you, thick scares you too — so how thick is \"just right\"?\n\nIn 2022, Min Byungsul's team at ISFH (the Institute for Solar Energy Research Hamelin, Germany) published a study in AIP Conference Proceedings that took this problem apart. They used **POLO passivating contacts — the academic name for what industry calls TOPCon, essentially an ultra-thin oxide plus doped polysilicon poly-Si/SiOx structure** — to isolate what's really going on.\n\n**The main takeaway isn't complicated: SiNx thickness and firing temperature are a matched pair. Change the thickness and you have to adjust the temperature. Move one without moving the other and either Voc drops or FF collapses.**\n\n## Technical Parameters\n\n### How the experiment was set up\n\nISFH used **p-type CZ wafers**, with an **n⁺ POLO contact** on the cell rear (tunnel oxide plus phosphorus-doped polysilicon).\n\nThe two key variables:\n\n1. **Rear SiNx capping thickness** — ranging from 40nm to 80nm\n2. **Peak firing temperature** — adjusted between 790°C and 810°C\n\nThey then measured two things: **contact resistivity ρc** (by TLM) and **cell IV parameters**.\n\nEarlier we looked at a 2016 JA Solar paper on how the **chemical composition** (Si/N ratio) of the **front-side** SiNx anti-reflection film affects silver paste contact. This 2022 ISFH work is about how the **physical thickness** of the **rear-side** SiNx capping affects silver paste contact. Put the two together and you cover both dimensions — \"chemical composition\" and \"physical thickness,\" front film and back film.\n\n### All samples fired at 800°C, only rear SiNx thickness varied\n\n| SiNx Thickness | Median ρc (800°C) | Status |\n| --- | --- | --- |\n| 40nm | ~1 mΩ·cm² | Very low |\n| 50nm | ~1.5 mΩ·cm² | Starting to rise |\n| 60nm | ~7 mΩ·cm² | Clearly rising |\n| 70nm | ~30-40 mΩ·cm² | Transition zone, steep climb |\n| 80nm | ~600 mΩ·cm² | Nearly 600x higher than at 40nm |\n\n### Firing temperature scan on 55nm and 60nm samples\n\n| Condition | Median ρc |\n| --- | --- |\n| 55nm SiNx + 800°C | 3.2 mΩ·cm² |\n| 60nm SiNx + 805°C | 2.8 mΩ·cm² |\n| 60nm SiNx + 810°C | 2.0 mΩ·cm² |\n\n## Technical Advantages\n\n### First finding: too thick and the paste can't fire through\n\nAll samples fired at a **800°C** peak, changing only the rear SiNx capping thickness. The pattern is clear from the table above — the amount of SiNx the paste can burn through during firing is limited. Cross that limit and the paste never reaches the polysilicon below, so contact resistance takes off.\n\nThe SEM images give direct evidence:\n\n- **40nm SiNx**: the paste fully burned through both the SiNx and the polysilicon, leaving plenty of **micron-scale etch pits** on the poly. The polysilicon was locally removed entirely — good contact, but the passivation layer got damaged.\n- **80nm SiNx**: only a tiny number of very small etch pits, no regions where the poly was fully removed — passivation held, but contact resistance was nearly 600x higher (about 2.8 orders of magnitude), and FF was basically wrecked.\n\n**ISFH's conclusion is blunt: there's an optimal SiNx window — between 50 and 60nm.** Too thin, the paste punches through the passivation and Voc craters. Too thick, the paste can't get through and contact resistance flies.\n\n### Second finding: thickness and temperature are paired\n\nISFH didn't stop at \"50-60nm is best.\" They asked a more practical shop-floor question: if the SiNx thickness changes, does the firing temperature need to change too?\n\nThey picked **55nm** and **60nm** groups and ran a temperature scan from **790°C to 810°C**.\n\nThe result is very clean:\n\n- **55nm SiNx**: FF peaks at **800°C**, best efficiency there. Go lower and the contact isn't good enough; go higher and passivation starts to suffer.\n- **60nm SiNx**: FF peaks at **805-810°C**. Because the SiNx is thicker, it needs a higher temperature for the paste to fire through.\n\nIn plain line terms: under these test conditions, going from 55nm to 60nm shifts the optimal firing temperature up by about 5-10°C. **That slope is only a reference for the same paste system — switch pastes and you need to re-calibrate.**\n\nThe contact resistivity data back this up too: higher temperature, better contact — as long as you don't cross the line where you start burning through the passivation.\n\n### The mechanism: etch pit size is the key\n\nISFH used SEM to lay out a very clear criterion:\n\n- **Pits larger than 1μm diameter**: poly fully removed, passivation damaged → **Voc drops**\n- **Pits smaller than 1μm diameter**: poly not fully removed, passivation intact → **contact resistance falls, Voc unchanged**\n\nISFH put it directly: \"a certain number of small-sized etch pits is necessary to form good contact. Etch pits below 1μm in diameter seem to have no effect on passivation quality.\"\n\n**Line criterion**: etch pits aren't better fewer, and aren't better more — the target is **small size, moderate distribution**. If you see lots of >1μm pits under the microscope, the temperature is too high or the SiNx too thin, and the passivation is already taking damage.\n\n## Product Application\n\n### What can a production line actually use?\n\n**1. SiNx thickness isn't better thin, and isn't better thick.** Below 40nm, the paste burns through the passivation and Voc craters; above 80nm, the paste can't fire through and contact resistance climbs nearly 600x.\n\n**2. Thickness and temperature are paired.** Change the SiNx thickness and the firing temperature has to follow. ISFH's data gives a reference — under these conditions, every extra 5nm of SiNx moves the peak temperature up about 5-10°C — **but re-calibrate after switching pastes.**\n\n**3. Etch pits are a \"window\" indicator.** Look at pit **size and density** by SEM and you can judge whether your current thickness-temperature combination sits inside the window. Lots of >1μm pits → too hot or film too thin; almost no pits → too cold or film too thick, contact may be a problem.\n\n**4. Back-film thickness also governs cosmetic yield, and paste selection.** The three points above are all about how thickness affects contact resistance and FF through the paste firing through or not. But on the line, rear SiNx thickness controls far more than electrical performance.\n\nIn real mass production, rear SiNx is typically controlled in the **70-85nm** range — thicker than the 50-60nm \"contact optimum\" in the ISFH paper. The reason is simple: the paper measured the pure contact optimum for its specific POLO structure and a particular paste, while a production line has to balance passivation, contact and color uniformity all at once, and picks a thicker, more stable range. **More importantly, commercial line pastes use a different glass-frit system than ISFH's lab paste, so the SiNx thickness window that can be burned through is different too.**\n\nChange the thickness and the refractive index changes, and the interference color of the film shifts with it. Too thin or too thick and the wafers show **color variation, off-color** and similar cosmetic downgrades that directly cut cosmetic yield. That in turn puts a hard requirement on the paste maker: **the paste must match the back-film process window**, not force the back film to accommodate one particular paste. Thickness and temperature must pair, and paste and film thickness must pair too — the line is a system, not a single-point tweak.\n\n### Three things the paper didn't say\n\n1. **The relation between POLO and TOPCon.** The POLO contact ISFH used is essentially ultra-thin oxide plus doped polysilicon (poly-Si/SiOx), basically the same as today's TOPCon rear structure, so the conclusions transfer directly. POLO is the academic name ISFH proposed; TOPCon is the industry-standard term; same structure at heart.\n2. **Paste model affects penetration depth.** Different pastes have different glass-frit compositions and can burn through different SiNx thicknesses. ISFH's 50-60nm is based on one specific paste — swap pastes and you may need to re-calibrate.\n3. **Long-term reliability isn't covered.** Will small etch pits grow into big ones over 25 years of outdoor aging? Will the interface degrade further under damp heat? The paper doesn't answer.\n\n### Reading it together with JA Solar 2016\n\n| Dimension | JA Solar 2016 | ISFH 2022 |\n| --- | --- | --- |\n| Application | Front SiNx anti-reflection film (ARC) | Rear SiNx capping layer |\n| Focus | Chemical composition of SiNx (Si/N ratio) | Physical thickness of SiNx |\n| Core variable | SiH₄/NH₃ gas ratio | SiNx thickness + firing temperature |\n| Failure mode | Off Si/N ratio → frit viscosity imbalance → high contact resistance | Wrong thickness → burn through or fail to burn through |\n| Fix direction | Tune the gas ratio to the optimal window | Pair thickness and temperature |\n| Shared mechanism | Frit-SiNx reaction kinetics decide contact quality | Frit-SiNx penetration depth decides contact quality |\n\nPut the two papers side by side and you get the full picture of front-film and back-film process: chemical composition decides whether you can contact well, physical thickness decides whether you hurt what's underneath while contacting.\n\n**[Nudge the coating Si/N ratio and Rs spikes, FF collapses, efficiency craters](https://mp.weixin.qq.com/s?__biz=MzkwOTQwMTI1Ng==&mid=2247487992&idx=1&sn=1c47bec2b7f8331fe2c63e811fc3928b&scene=21#wechat_redirect)**\n\n### A reminder for the line: don't only stare at poly when hunting for efficiency loss\n\nWith both papers done, back to our own line. When chasing efficiency loss, an engineer's reflex is to first check rear poly thickness, doping level, tunnel oxide thickness — their impact on FF and Voc is well understood and these are standard check items. But the **rear SiNx capping layer** often gets waved off as a \"passivation/cosmetic layer,\" and few people think of it in terms of contact resistance.\n\nThe value of this ISFH paper is exactly that it drags this overlooked variable back onto the table: **wrong back-film thickness, paste doesn't fire through or burns through, and FF collapses all the same.** Next time you hit a \"poly parameters untouched, yet FF mysteriously dropped\" situation, don't just circle around the poly — go back and check whether back-film thickness and firing temperature still pair.\n\nWorth noting: ISFH's experiment is based on conventional firing. The LECO technology now widely adopted on lines can optimize contact through a subsequent laser/current step, which to some extent reduces sensitivity to the firing-temperature-thickness pairing — but back-film thickness is still the base window and can't be ignored.\n\n### Ooitech's View\n\nWe see the same thing on every TOPCon line we commission — the rear SiNx capping gets treated as just a color film, and then FF quietly slips with nobody checking the thickness-temperature pairing. The ISFH data lines up with what pushes people toward LECO, since decoupling contact formation from the firing step buys real margin when your paste's frit chemistry and your back-film window don't perfectly agree. If you want to see how these steps play out on a real module line — coating, firing, stringing and all — the Ooitech YouTube channel at [www.youtube.com/ooitech](http://www.youtube.com/ooitech) is worth a follow. And keep in mind this is a cell-level study; the module line inherits these cells but the contact fate is already sealed upstream.\n\n## References\n\n- Min B. et al., AIP Conf. Proc. 2487, 020014 (2022) (DOI: 10.1063/5.0089239)\n- Chen X.Y. et al., Solar Energy 126 (2016) 105–110 (DOI: 10.1016/j.solener.2016.01.001)\n\n## Further reading and background data\n\nPublic reference material on this topic, published by the organisations that maintain the industry's technology roadmap and market data:\n\n- [VDMA — International Technology Roadmap for Photovoltaic (ITRPV)](https://www.vdma.org/international-technology-roadmap-photovoltaic)\n- [Fraunhofer ISE — Photovoltaics Report](https://www.ise.fraunhofer.de/en/publications/studies/photovoltaics-report.html)\n- [U.S. Department of Energy — Photovoltaics](https://www.energy.gov/eere/solar/photovoltaics)\n\n---\n\n##### Tags :\n\n![](/template/ooitech/assets/img/shape/06.png)\n\n![](https://cdn.ooitech.com/runtime/image/w800_h700_fitblur_v2_w800_h700_fitblur_v2_1757399770541443.webp)\n\n### Request A Quote\n\nAll uploads are secure and confidential.\n\n## We deliver expertise you can trust our service\n\nDirect-from-Factory Equipment.\n\n![](/template/ooitech/assets/img/icon/money-2.svg)\n\n### Cost-Effective Advantages\n\nWe deliver exceptional value, maximizing results while optimizing budgets for clients.\n\n![](/template/ooitech/assets/img/icon/staff.svg)\n\n### Our Experience Team\n\nOur skilled professionals specialize in innovative solutions and tailored strategies.\n\n![](/template/ooitech/assets/img/icon/certified.svg)\n\n### 15+ Years Industry Experience\n\nDeep expertise ensures reliable, trend-aware, and proven outcomes for success.\n\n![](https://cdn.ooitech.com/static/upload/image/20250910/1757477357667605.webp )\n\n![](https://cdn.ooitech.com/static/upload/image/20250910/1757477724911512.webp)\n\n![](/template/ooitech/assets/img/shape/06.png)\n\n## What Our Client Say's about us\n\nClient testimonials praise our deep understanding of their challenges, which leads to innovative solutions and strong ROI. Long-term collaborations—some over a decade—demonstrate their trust and satisfaction. Their success stories drive us to continually exceed expectations. [Know More **](#quote-form)\n\n![](/template/ooitech/assets/img/icon/quote.svg)\n\nThanks to Ooitech for providing the fully automated production equipment—your installation and after-sales service have been excellent.\n\n![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026041720921238.webp)\n\n### Amjad\n\n![](/template/ooitech/assets/img/icon/quote.svg)\n\nthank you for ooitech's professional support and on time after service.\n\n![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1784509010217979.webp)\n\n### Diarra From Africa\n\n![](/template/ooitech/assets/img/icon/quote.svg)\n\nThanks to Ooitech for providing highly suitable BC solar cell experimental equipment.\n\n![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1776426122864564.webp)\n\n### KTECH\n\n![](/template/ooitech/assets/img/icon/quote.svg)\n\nThank you again so much again for the very big big help for improving and fixing the factory and also teaching the workers how to use the machines\n\n![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1757479675272137.webp)\n\n### Mark\n\nBIPV Philippines\n\n![](/template/ooitech/assets/img/icon/quote.svg)\n\nA man with a big soul. Thank you very much for your visit Mr Wu. Thank you very much for the services provided in installing equipment and training my students. The kindest person and professional in his field\n\n![](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026041716444445.webp)\n\n### Jizzakh Polytechnic Institute\n\n## Our Latest Products\n\n![SS-1500B Solar Cell Tabber Stringer: 1200 Cells/h](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774253968620270.webp)\n\n- [** ooitech](./SS-1500B-Automatic-Solar-Cell-Welding-Machine-High-Speed-Tabber-Stringer-for-BC-TOPCON-PERC-Cells.html)\n- [** 84709](./SS-1500B-Automatic-Solar-Cell-Welding-Machine-High-Speed-Tabber-Stringer-for-BC-TOPCON-PERC-Cells.html)\n\n### SS-1500B Solar Cell Tabber Stringer: 1200 Cells/h\n\nSS-1500B automatic solar cell welding machine by Ooitech - High-performance tabber stringer for BC, TOPCON, PERC\n\n![OPT-S110H Offline String EL Tester: ≤2s, 4.6MP](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774350940561245.webp)\n\n- [** Rachael](./offline-string-el-tester-opt-s110h-solar-cell-string-electroluminescence-testing-equipment-ooitech.html)\n- [** 88440](./offline-string-el-tester-opt-s110h-solar-cell-string-electroluminescence-testing-equipment-ooitech.html)\n\n### OPT-S110H Offline String EL Tester: ≤2s, 4.6MP\n\nOPT-S110H Offline String EL Tester from Ooitech delivers high-speed electroluminescence inspection for solar cell strings up to 1250mm.\n\n![OEL-S2400 Solar Panel EL Tester: 4928 x 3264px](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774351284414161.webp)\n\n- [** Rachael](./solar-panel-el-defect-tester-oel-s2400-electroluminescence-testing-machine-for-solar-module-quality-inspection.html)\n- [** 60854](./solar-panel-el-defect-tester-oel-s2400-electroluminescence-testing-machine-for-solar-module-quality-inspection.html)\n\n### OEL-S2400 Solar Panel EL Tester: 4928 x 3264px\n\nOoitech OEL-S2400 Solar Panel EL Defect Tester is an offline electroluminescence testing machine designed to detect microcracks, black spots\n\n![Solar Panel Sealant and Tape: Silicone, Butyl, PET](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_2026032711586064.jpg.webp)\n\n- [** Rachael](./PV-Module-Sealant-Tape-Solutions-Essential-Components-for-Solar-Panel-Reliability.html)\n- [** 73323](./PV-Module-Sealant-Tape-Solutions-Essential-Components-for-Solar-Panel-Reliability.html)\n\n### Solar Panel Sealant and Tape: Silicone, Butyl, PET\n\nSolar panel sealant and tape for module assembly: silicone frame sealant, butyl tape and busbar insulation tape, UV-resistant for 25-year outdoor exposure.\n\n![KS-01C Junction Box Welding Machine: 16s Cycle](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774492507915923.webp)\n\n- [** Rachael](./junction-box-welding-machine-ks-01c-automatic-solar-panel-junction-box-soldering-equipment-ooitech.html)\n- [** 92564](./junction-box-welding-machine-ks-01c-automatic-solar-panel-junction-box-soldering-equipment-ooitech.html)\n\n### KS-01C Junction Box Welding Machine: 16s Cycle\n\nOoitech KS-01C Junction Box Welding Machine features automatic hot bar tin welding and high frequency welding with CCD positioning accuracy of ±0.1mm.\n\n![SS-2500B Tabber and Stringer: 2400 Cells/h, 3-20BB](https://cdn.ooitech.com/runtime/image/w800_h600_fitblur_v2_1774258018905303.webp)\n\n- [** ooitech](./SS-2500B-Full-Automatic-Solar-Cell-Tabber-Stringer-Machine-High-Speed-Production-Line-Equipment.html)\n- [** 37084](./SS-2500B-Full-Automatic-Solar-Cell-Tabber-Stringer-Machine-High-Speed-Production-Line-Equipment.html)\n\n### SS-2500B Tabber and Stringer: 2400 Cells/h, 3-20BB\n\nSS-2500B full automatic tabber stringer machine for crystalline silicon solar cells with 2400PCS/H capacity, featuring infrared soldering\n",
    "endpoints": {
        "html": "https://www.ooitech.com/sinx-too-thin-and-silver-paste-punches-through-the-poly-layer-too-thick-and-contact-resistance-jumps-600x-isfh-points-to-a-fix.html",
        "markdown": "https://www.ooitech.com/sinx-too-thin-and-silver-paste-punches-through-the-poly-layer-too-thick-and-contact-resistance-jumps-600x-isfh-points-to-a-fix.md",
        "agentManifest": "https://www.ooitech.com/.well-known/agent.json",
        "llmsTxt": "https://www.ooitech.com/llms.txt",
        "sitemap": "https://www.ooitech.com/sitemap.xml",
        "quote": "https://m.ooitech.com/api/quote.php"
    }
}